Cold Heading7 min read

Bolt Shank Scoring in Cold Heading

By Jake Wang, Overseas Sales Manager ·

A straight mark on a bolt shank can survive several forming stations. The die that releases the finished blank may have had nothing to do with it. Before ordering a replacement cold heading die, find the first stage where the line appears. Keep a piece of incoming wire, a cut blank and the formed samples from the same coil and run. A line already on the wire, a groove added by the feed path and a mark made during extrusion call for different work.

Follow the shank from coil to finished blank

Start with the drawing. Circle the affected band and measure its distance from a feature you can find again, such as the under-head face on the formed blank. On a stepped shank, mark whether the line ends at the change in diameter or continues beyond it. Photograph the whole part first, then photograph the line with a scale under angled light. Keep a sound piece from the same setup beside it. A spot that looks like a groove under one light may simply reflect differently as you turn the part.

Work backwards through the route. Keep incoming wire taken before it touches the feed hardware, wire or a cut blank from after feeding, and parts from immediately before and after the station that forms the affected diameter. If the mark was found after thread rolling, coating or bulk handling, include a sample from just before that operation as well. Collect and inspect samples under the site's approved setup and isolation procedures. Label the coil, station, sample order and tooling ID. Where the machine preserves orientation, add a station reference to the photos. When blanks can rotate in transfer, use the axial location and stage history and leave the angular match open.

A smooth-looking wire sample also has limits. Carpenter Technology's cold forming guide treats billet surface soundness and wire condition as inputs to headability. If a line is already present on representative incoming wire, retain the material and ask the wire supplier how to classify it. A visual check may locate an indication. Depth or an opening below the surface may require examination under the applicable inspection procedure.

What each sample can tell you

First appearance of a shank mark and what to check next
What you seeWhat to compareWho should act first
A line is visible on incoming wire before the feederCompare retained wire from the suspect coil with a known-good coil. Keep the lot IDs and ask how the discontinuity will be examined.Incoming quality and the wire supplier. Hold the affected lot for disposition under the agreed rules.
The line first appears after feeding or on the cut blankExamine guide and feed contact points and the cut-off tooling. A mark confined to the cut face is a separate observation from one along the outside diameter.The setup team. Isolate the suspect contact before opening a die replacement request.
A repeated line first appears on the reduced diameter after extrusionMatch the axial band on the part to the tool drawing. Inspect the approach and sizing land for adherent material or tool damage before cleaning. Record the tool's installed orientation if it can be traced.Tooling and process engineering. Preserve the tool and samples so the supplier can review geometry and the contact surface.
The headed blank is clean and the line appears laterCompare clean retained blanks with samples immediately after rolling, finishing or handling, one step at a time.The owner of the first affected downstream step. Keep the heading die in the investigation only if the evidence leads back to it.

A raised deposit on the die and a groove on the part make material transfer a reasonable working explanation. Photograph the deposit before removal so the toolmaker can see the location. A nick, exposed substrate or a mark on the opposing machine contact can look similar in a phone photo. If the surface is critical, ask how the technician will distinguish a removable deposit from loss of tool material and confirm the condition of the sizing diameter afterward.

Why one bright streak need not mean galling

A 2026 upsetting and forward extrusion experiment used JIS SCr415H steel with a zinc phosphate and reactive soap coating. The authors observed galling in the tapered region of one test geometry. In the other geometry they found a bright region with evidence consistent with coating damage and local exposure of the steel, without severe galling. The comparison is useful because a bright streak and severe galling were distinguishable on those samples. Their trial geometries and materials define the scope of the result. They establish neither a shop acceptance limit nor a prediction of die life for a different part.

Published test results for coated JIS SCr415H steel
Test after upsettingInferred friction coefficient (dimensionless)Surface observation
UP–RC≈0.04Galling in the tapered region.
UP–WC≈0.04Local metallic sheen consistent with coating damage. No severe galling reported in that region.

The two inferred coefficients are similar even though the local surface observations differ. Use the photos and the stage history when asking the supplier to assess a particular mark.

Example: the mark is already present before the first die

A stepped bolt returns from final inspection with a thin line on the larger shank diameter. The smaller extruded diameter looks clean. The retained wire from before the feeder looks clean, too. The same line is visible on the outer surface of several cut blanks, at an axial position that survives into the larger diameter. That moves the first examination to the path between the retained wire sample and the cut blank. Record which guides and feed components were installed, and inspect them and the cut-off tooling during an approved stop. A line on the outside diameter and a burr around the perimeter of the cut face should be photographed separately.

After an approved correction, compare a newly cut blank with one taken before the correction and follow both conditions to the final blank. If the new cut blanks are clean and the finished blanks still show the line, resume the comparison at the next station. If both are clean under the agreed inspection, the result supports the feed-path investigation and gives purchasing a reason to hold off on a die order. If the samples could not be tied to the same coil or setup, record that gap before drawing a conclusion.

Specify what the supplier should check

For a die review, send the current part and tool drawing revisions, a marked section through the affected diameter, wire grade and lot, wire surface preparation, the station sequence, tool identification, and indexed photos of sound and affected parts. If the groove affects a seal or sliding fit, show the functional band and the drawing requirement. A general roughness reading and the depth of an isolated groove answer different questions. State which one governs acceptance and where it is measured. For covered bolts, screws and studs, ISO 6157-1 describes the scope for surface discontinuities. Confirm the standard, edition and any drawing-specific criteria that apply to the order.

Carbide die core for bolt tooling from the Jungu catalogue
Jungu catalogue photo of a carbide die core for bolt tooling.

Review the carbide die core for bolt tooling and the bolt and screw forming die range. The carbide die polishing guide covers how to preserve the working profile once the contact surface has been identified. Send your drawing and marked samples for a die review.