Nut Forming Dies7 min read

Nut Forming Dies: Where to Look When Piercing Leaves a Burr

By Jake Wang, Overseas Sales Manager ·

When nut forming dies produce a blank with a burr on just one side of the pierced hole, keep the preform, the pierced blank and the ejected slug from the same short trial. A burr that repeats at one angular position gives you a place to look. The mark alone cannot tell you whether the material entering the piercing station was off centre, a cutting edge was damaged or the removed slug stayed in the tool.

This guide applies to cold-formed through-hole nut blanks in which a punch removes the remaining web. Use it before tapping or deburring changes the edge you need to inspect. The intermediate drawing and agreed inspection plan govern release. Set aside suspect parts under that plan while you compare the evidence.

Put the burr and the preform on the same reference

Collect a preform immediately before piercing and a blank immediately after it. Where practical, also keep a known acceptable blank from the same drawing revision and material condition. Identify the piercing direction, place the exit face upwards and mark one nut flat as your orientation reference. If a transfer turns the part over between stations, record the turn so both samples can be related to the same flat. A loose slug can lose its orientation. Record its shape and sequence where you can establish them, and leave the angular position unknown if you cannot.

Record the burr height from the adjacent specified reference surface at labelled positions around the hole. A profile across a chamfer can include the intended slope. Mark the section and zero surface on the inspection sketch and use the same method for the comparison blank. Keep the individual readings before calculating a maximum or spread. If the feature is too small for the method to resolve, ask inspection for a suitable measurement before changing tooling.

Read both sides of the last unpierced web

The web is the material left between the opposing recesses before the punch opens the hole. On a spare preform, measure the recess locations relative to the agreed outside reference. A section or other suitable inspection can show where the web sits and whether thickness varies across it. Use more than one direction if the first section cannot establish the pattern. A hole diameter measured after piercing cannot show where the unpierced web lay.

In Hsia and Shih's six-stage study of a C1010 long hex flange nut, the authors planned the lead recess in the flange-forming stage to keep the subsequent recess aligned and reduce the risk of burrs from off-centre piercing. Examine the upstream preform before asking a supplier to alter the last punch. The paper describes a particular process. Use your own stage sequence and acceptance criteria.

Choose the inspection and the parts to quote

From burr pattern to tooling review
Evidence from the trialNext checkQuotation decision
The high burr and displaced preform recess repeatedly face the same flatCompare recess location and web section before piercing. Confirm the recorded transfer orientation.Review the upstream preform and its locating tool before quoting a piercing-only change.
The preform passes its checks and the burr repeats at one tool orientationCompare the punch edge and opposing support or cutting insert with the approved assembly. Look for matching damage or seating marks.Ask for a punch-only quote if the opposing component and fit can be confirmed. Include both parts for review if they cannot.
The mark comes and goes, or a slug is found where it should have clearedRecord the affected part sequence and slug recovery point. Compare with the documented discharge path.Include the discharge components in the review before ordering a new cutting edge.
Burr height rises around most of the rim over the runCompare early and late samples, tool edge condition and material lot. Use the same height reference and inspection method.Ask the supplier to evaluate edge condition and the paired tool before treating it as local misalignment.

Advanced Cold Forming's tooling notes describe several slug-discharge arrangements. Some retain the slug mechanically and others assist its removal with air. Identify the arrangement on your station drawing before comparing the discharge count with the number of strokes. A slug retained by design can be released on a later stroke. If there are signs of a blockage or unexpected retention, have qualified setup staff inspect it using the machine manufacturer's procedures and the plant's safety rules.

A local increase and a rim-wide increase lead to different checks

Suppose an acceptable comparison blank reads 0.02 mm at both a marked flat and the opposite side of the exit rim. A suspect blank reads 0.10 mm and 0.03 mm at those same positions. The difference across the suspect blank is 0.07 mm. The readings indicate where to take a section or make a repeat measurement. These illustrative values establish neither a burr tolerance nor the cause of the defect.

On the next available samples, compare the same positions with the web section on matching preforms. If the offset repeats before piercing, check where it first appears in the sequence. If preforms are consistent and the high reading follows one installed tool position, compare the supported assembly and look for a matching edge or seat mark. The quality team should use the approved drawing and measurement uncertainty for lot decisions. Preserve the parts before polishing away the evidence.

What should go with a request for replacement tooling?

Send the finished-nut and intermediate drawings, machine and station, piercing assembly section, and material and tool IDs. Attach preform and pierced-blank measurements with the orientation marked. Include the slug record or state why it could not be tied to the sample sequence. Highlight the components you will reuse and ask the supplier to state which interfaces and trial samples the quote covers. For approval of the blank handed to threading, see the pre-tapping hole inspection guide.

Jungu catalogue set of nut and bolt punch and die components
A punch and die set from Jungu's catalogue. Mark the piercing station and individual components on the assembly drawing for your order.

See Jungu's carbide nut forming die and hex nut punch and die set. Send the station drawing and labelled trial evidence for a tooling quotation.